ISG PLATE PROPRIETARY GRADES

SPECIFICATION SPA-90* T-1®* T-1® Type A* T-1® Type B* T-1® Type C* Lukens® 130* Lukens® 690Z*▲
Type of Steel Alloy Alloy Alloy Alloy Alloy Alloy
Requirements for Delivery A6, A20** A6, A20** A6, A20** A6, A20** A6, A20** A6
Tensile Strength (ksi) 110/130 to 110/130 110/130 110/130 110/130 to Info. only 110/136
2 1/2" incl.; 2 1/2" incl.;
100/130 100/130
over 2 1/2" over 2 1/2"
Yield Strength (Min. ksi) 100 to 2 1/2" 100 100 100 100 to 2 1/2" 130 100
(Yield Point if incl.; 90 incl.; 90
designated YP) over 2 1/2" over 2 1/2"
Spec. Thickness (Max. in.) 8 2 1/2 11/4 2 6 2 6.5
ISG Plate
Thickness (Max. in.) 8 2 1/2 11/4 2 6 Refer to 4 6.5
Chemical Composition (%) Unless a range is specified, individual values are maximums
Carbon .14/.21 .10/.20 .12/.21 .12/.21 .14/.21 .12/.18 .15
Manganese .95/1.30 .60/1.00 .70/1.00 .95/1.30 .95/1.30 1.55 1.25
Phosphorus .035 .035 .035 .035 .035 .025 .015
Sulfur .040 .040 .040 .040 .040 .003 .005
Silicon .15/.35 .15/.35 .20/.35 .20/.35 .15/.35 .15/.50 .15/.55
Chromium 1.00/1.50 .40/.65 .40/.65 .40/.65 1.00/1.50 .65 .70
.80 if
approved
by customer
Nickel 1.20/1.50 .70/1.00 - .30/.70 1.20/1.50 1.00 1.0/3.5
Molybdenum .40/.60 .40/.60 .15/.25 .20/.30 .40/.60 .60 .70
Copper ■ .15/.50 .20/.40 .20/.40 ■ - .30
if specified if specified
Other Elements .03/.08 V .03/.08 V .03/.08 V .03/.08 V .03/.08 V .08 V, CT .005B
.0005/.006 B .01/.03 Ti .0005/.005 B .04 Cb .04Ti
.005 B .08 V
Heat Treatment Required Q&T Q&T Q&T Q&T Q&T Q&T Q&T
Remarks LCVN LCVN
* It is important to note that this grade of steel may be susceptible to cracking in the heat-affected zone of welds during post-weld
heat treatment (stress relief). Therefore, ISG Plate recommends that careful consideration be given to this phenomenon by
competent welding engineers before stress relieving is applied to weldments of this grade. Also, it is not recommended for
service at temperatures lower than -50˚F or higher than 800˚F.
** A20: Raise tensile strength range by 5 ksi.
† Post-weld heat treatment may degrade heat-affected zone strength and toughness. Pretesting of specific welding and post-weld
heat treating procedures is recommended to assure optimization of final property levels.
▲ Also available as ABS grades EQ/FQ 63/70
■ Restricted to ASTM A20 limits for unspecified elements.

T-1 Brochure
Lukens 130 Brochure
Lukens 690Z Brochure

35
CON TINUED ISG PLATE PROPRIETARY GRADES

RQC-60 RQC-60
SPECIFICATION (Q&T) (N) RQC-80 RQC-90 RQC-100 Spartan® I††
Type of Steel Carbon Carbon Carbon Carbon Carbon Alloy
Requirements for Delivery A6 A6 A6 A6 A6 A6, A20
Tensile Strength (ksi) 80/100 to 70/90 to 95 100 110 60/110*
21/2" incl.; 21/2" incl.; available
75/95 over 65/85 over
21/2" 21/2"
Yield Strength (Min. ksi) 60 to 21/2" 50 to 21/2" 80 90 100 50/100*
(Yield Point if incl.; 55 incl.; 45 available
designated YP) over 21/2" over 21/2"
Spec. Thickness (Max. in.) - - - - - -
ISG Plate
Thickness (Max. in.) 4 4 11/2 11/2 11/4 4**

Chemical Composition (%) Unless a range is specified, individual values are maximums
Carbon .21 .21 .21 .21 .21 .07
Manganese .70/1.35 to .70/1.35 to 1.35 1.35 1.50 .40/.70
11/2" incl.; 11/2" incl.;
1.00/1.60 1.00/1.60
over 11/2" over 11/2"
Phosphorus .035 .035 .04 .04 .04 .015
Sulfur .04 .04 .05 .05 .05 .005
Silicon .50 .50 .40 .40 .40 .40
Chromium - - - - - .60/.90
Nickel - - - - - .70/1.00
Molybdenum - - - - - .15/.25
Copper .35 .35 .35 .35 .35 1.00/1.30
Other Elements .0005 Min. B .0005 Min. B .0005 Min. B .0005 Min. B .0005 Min. B .02/.06 Cb
CT
Heat Treatment Required Q&T N Q&T Q&T Q&T As rolled
&PHT,
N&PHT
or Q&PHT
* These minimum strength levels are available depending on heat treatment, thickness and toughness requirements.
Consult ISG Plate for specific available requirements.
** Consult ISG Plate for plates over thickness noted or additional chemistries.
†† It is important to note that this grade of steel may be susceptible to cracking in the heat-affected zone of welds during post-weld
heat treatment (stress relief) or elevated temperature service. Also, post-weld heat treatment or elevated temperature service
may degrade heat affected zone toughness. Therefore, ISG Plate recommends that careful consideration be given to these
phenomena by competent welding engineers before application.

Spartan Brochure

36
CON TINUED ISG PLATE PROPRIETARY GRADES
Duracorr®▲ Duracorr®▲ Duracorr®
SPECIFICATION Spartan II††
®
Spartan III††
®
Grade 40 Grade 50 300
Type of Steel Alloy Alloy Stainless Stainless Stainless
Requirements for Delivery A6, A20 A6, A20 A480 A480 A480
Tensile Strength (ksi) 90/110* 100/130* 66 Min. 70 Min. -
available available
Yield Strength (Min. ksi) 80/100* 90/120* 40 50 -
(Yield Point if available available
designated YP)
Spec. Thickness (Max. in.) - -
ISG Plate
Thickness (Max. in.) 4** 4** 4 4 4
Chemical Composition (%) Unless a range is specified, individual values are maximums
Carbon .07 .07 .025 .025 .025
Manganese .75/1.15 .75/1.15 1.50 1.50 1.50
Phosphorus .015 .015 .040 .040 .040
Sulfur .005 .005 .015 .015 .015
Silicon .40 .40 .70 .70 .70
Chromium .45/.75 .45/.75 11.0/12.50 11.0/12.50 11.0/12.50
Nickel 1.50/2.00 3.35/3.65 1.00 1.00 1.00
Molybdenum .30/.55 .55/.65 .20/.30 .20/.30 .20/.30
Copper 1.00/1.30 1.15/1.75 - - -
Other Elements .02/.06 Cb .02/.06 Cb .030 N .030 N .030 N
Heat Treatment Required Q&PHT Q&PHT Tempered Tempered -
Remarks 233 Max. Surf. HB - 260/360 HB
▲ Also available as ASTM A1010.

* These minimum strength levels are available depending on heat treatment, thickness and toughness requirements.
Consult ISG Plate for specific available requirements.
** Consult ISG Plate for plates over thickness noted or additional chemistries.
†† It is important to note that this grade of steel may be susceptible to cracking in the heat-affected zone of welds during post-weld
heat treatment (stress relief) or elevated temperature service. Also, post-weld heat treatment or elevated temperature service
may degrade heat affected zone toughness. Therefore, ISG Plate recommends that careful consideration be given to these
phenomena by competent welding engineers before application.

Spartan Brochure
Duracorr Brochure
Duracorr 300 Brochure

37
CON TINUED ISG PLATE PROPRIETARY GRADES

BethStar® BethStar® BethStar® BethStar® V-Star® V-Star® T-Star®* T-Star®*


SPECIFICATION Grade 50 Grade 60 Grade 70 Grade 80 Grade 50 Grade 65 Grade 42 Grade 50
Type of Steel HSLA HSLA HSLA HSLA HSLA HSLA HSLA HSLA
Requirements for Delivery A6 A6 A6 A6 A6 A6 A6 A6
Tensile Strength (ksi) 60 Min. 70 Min. 80 Min. 90 Min. 65 Min. 80 Min. 60 Min. 65 Min.
Yield Strength (Min. ksi) 50 60 70 80 50 65 42 YP 50YP
(Yield Point if
designated YP)
-
Spec. Thickness (Max. in.) - - - - - - -
ISG Plate
Thickness (Max. in.) 2 1/2 11/2 1 3
/4 .875 1
/2 2 2
Chemical Composition (%) Unless a range is specified, individual values are maximums
Carbon .10 .10 .10 .10 .10 .10 .12 .12
Manganese 1.65 1.65 1.65 1.65 1.45 1.50 1.35 1.35
Phosphorus .025 .025 .025 .025 .025 .025 .025 .025
Sulfur .010 .010 .010 .010 .010 .010 .018 .018
Silicon .35 .35 .35 .40 .25/.40 .25/.40 .40 .40
Vanadium .10 .10 .10 .10 .10 .10 .04 .04
Columbium .06 .06 .06 .06 - - - -
Titanium - - - - - - .02 .02
CE (IIW) .27/.31 .28/.32 .30/.34 .37/.41 .38 .38 .35 .35
PCM .16/.18 .16/.18 .16/.19 .21/.24 .22 .22 .20 .20
Remarks - - - - TMCP TMCP TMCP TMCP
CE (IIW) = C + Mn /6 + (Cr+Mo+V)/5 + (Cu+Ni)/15
PCM = C + (Mn+Cu+Cr)/20 + Mo /15 + V/10 + Si /30 + Ni /60 + 5B

* Also available as A572 Type 5.


▲ In the future the HY and HSLA Navy Alloy grades will be specified by the NAVSEA Technical Publication T9074-BD-GIB-010/0300
replacing the MIL-S Specifications. The information given here is from this new document.

▲▲ ISG Plate declared chemistries

†† It is important to note that this grade of steel may be susceptible to cracking in the heat-affected zone of welds during post-weld
heat treatment (stress relief) or elevated temperature service. Also, post-weld heat treatment or elevated temperature service
may degrade heat affected zone toughness. Therefore, ISG Plate recommends that careful consideration be given to these
phenomena by competent welding engineers before application.

BethStar Brochure
T-Star Brochure
Military Alloy Brochure

38

Vous aimerez peut-être aussi